🖨 Print 📄 Download PDF

KELUM® Aluminium Hydroxide — Flame Retardant Testing

Hanzhong Delike New Materials Co., Ltd.
FLAME RETARDANT TESTING
Document No: AL-FRT-2026-01
Revision: 1.0 | Effective: July 2026
Page 1 of 1

1. Flame Retardant Mechanism — Endothermic Decomposition

KELUM® Aluminium Hydroxide [Al(OH)₃] is a halogen-free, environmentally friendly inorganic flame retardant that functions through an endothermic decomposition mechanism. When exposed to heat in the range of 250–350 °C, Al(OH)₃ undergoes thermal decomposition, absorbing a significant amount of energy (approx. 1,050 J/g) from the combustion zone. This endothermic reaction cools the substrate below its ignition temperature, effectively suppressing flame propagation.

Thermal Decomposition Reaction:
2 Al(OH)₃  →  Al₂O₃  +  3 H₂O ↑
Endothermic enthalpy: ~1,050 J/g  |  Water release: 34.5% by mass  |  Onset: 250 °C  |  Peak: 300–320 °C

The released water vapor (H₂O) serves three critical functions simultaneously: (1) it dilutes combustible gases in the flame zone, reducing the concentration of flammable volatile compounds; (2) it forms a protective steam blanket that displaces oxygen from the polymer surface; and (3) the residual alumina (Al₂O₃) creates a thermally stable, insulating char layer that acts as a barrier to heat and mass transfer. Unlike halogenated flame retardants, KELUM® Al(OH)₃ generates no toxic or corrosive gases, produces extremely low smoke, and leaves no hazardous decomposition products — making it the preferred choice for low-smoke, zero-halogen (LSZH) cable compounds, construction materials, and public-transport interior applications.


2. Standard Flame Retardant Tests

The flame retardant performance of KELUM® Al(OH)₃ in polymer matrices is evaluated according to the following internationally recognized test standards. Results are dependent on loading level, polymer matrix, and compound formulation.

Test Standard Full Name Key Metrics Description & Relevance Typical KELUM® Result
UL 94 Standard for Safety — Flammability of Plastic Materials V-0 / V-1 / V-2 Rating Vertical burn test measuring afterflame time, afterglow, and flaming drips. The most widely referenced plastics flammability standard worldwide. V-0 (at ≥ 60% loading in EVA/PE)
LOI
ISO 4589 / ASTM D2863
Limiting Oxygen Index O₂ % required to sustain combustion Measures the minimum oxygen concentration in an O₂/N₂ mixture that supports candle-like combustion. Higher values indicate better flame retardancy. Materials with LOI > 21% are considered "self-extinguishing" in air. ≥ 28% (neat KELUM® in EVA)
Cone Calorimeter
ISO 5660 / ASTM E1354
Cone Calorimeter — Heat Release & Smoke HRR, THR, SEA, TTI, MLR Bench-scale fire test that measures heat release rate (HRR), total heat release (THR), specific extinction area (SEA / smoke), time to ignition (TTI), and mass loss rate (MLR) under a controlled radiant heat flux (typically 35 or 50 kW/m²). pHRR reduced by 50–70%
vs. unfilled polymer
TGA / DSC Thermogravimetric Analysis / Differential Scanning Calorimetry Tonset, Tpeak, ΔH, Residue Thermal analysis techniques characterizing decomposition temperature, mass loss profile, and endothermic enthalpy. TGA quantifies decomposition steps; DSC measures the energy absorbed during the endothermic transition. Tonset: 250 °C
Tpeak: 300–320 °C
ΔH: ~1,050 J/g

HRR = Heat Release Rate (peak & average)  |  THR = Total Heat Release  |  SEA = Specific Extinction Area (smoke density)  |  TTI = Time to Ignition  |  MLR = Mass Loss Rate  |  Results are formulation-dependent. Contact our technical team for grade-specific data.


3. Test Methodology

All flame retardant testing is conducted under controlled laboratory conditions in accordance with the applicable ISO, ASTM, and UL standards. Below are the standardized procedures for each test method.

UL 94 — Vertical Burn Test (V-0 / V-1 / V-2)

  • Specimen: 125 × 13 × thickness mm bars (typically 1.6 or 3.2 mm)
  • Conditioning: 48 h at 23 ± 2 °C, 50 ± 5 % RH; plus 168 h at 70 °C for elevated-temperature conditioning
  • Procedure: Specimen clamped vertically; 20 mm Bunsen burner flame (50 W, methane) applied to bottom center for 10 s, removed; afterflame time t₁ recorded; flame reapplied for 10 s; afterflame + afterglow t₂ recorded
  • Cotton indicator: Surgical cotton placed 300 mm below specimen to detect flaming drips
  • Criteria (V-0): t₁ + t₂ ≤ 10 s per specimen; total ≤ 50 s for 5 specimens; no flaming drips; no afterglow exceeding 30 s
  • Standard: UL 94, 6th Ed. / IEC 60695-11-10 / GB/T 2408

LOI — Limiting Oxygen Index (ISO 4589 / ASTM D2863)

  • Specimen: 80–150 × 10 × 4 mm bars (Type IV)
  • Conditioning: 24 h at 23 ± 2 °C, 50 ± 5 % RH
  • Procedure: Specimen mounted vertically in a glass chimney; O₂/N₂ mixture flows upward at 40 ± 2 mm/s; top-ignited with a pilot flame; O₂ concentration adjusted in steps until the minimum concentration sustaining 3-minute or 50 mm burn is found
  • Measurement: LOI = O₂ vol% at which combustion is just sustained. Higher LOI → better flame retardancy. Materials with LOI < 21 burn readily in air.
  • Relevance: Widely used in cable and wire industries; specified in many product standards (e.g., IEC 60332, EN 50399)

Cone Calorimeter (ISO 5660-1 / ASTM E1354)

  • Specimen: 100 × 100 × up to 50 mm plaque; tested in horizontal orientation with retainer frame and grid
  • Conditioning: To constant mass at 23 ± 2 °C, 50 ± 5 % RH
  • Heat flux: Typically 35 or 50 kW/m²; specimen positioned 25 mm below cone heater (or 60 mm for some applications)
  • Measured parameters: Heat Release Rate (HRR, kW/m²) — peak (pHRR) and average over test duration; Total Heat Release (THR, MJ/m²); Specific Extinction Area (SEA, m²/kg) — smoke production; Time to Ignition (TTI, s); Mass Loss Rate (MLR, g/s·m²); CO/CO₂ yield (kg/kg)
  • Data collection: Oxygen consumption calorimetry; at least 3 replicates; test duration until flameout or 20–30 min
  • Significance: Considered the best single bench-scale predictor of real fire behavior

TGA / DSC — Thermal Analysis

  • TGA Sample: 5–15 mg powder in alumina or platinum crucible
  • TGA Conditions: N₂ or air atmosphere; heating rate 10, 20, or 40 °C/min (typically 20 °C/min); temperature range: ambient to 800–1000 °C
  • TGA Output: Mass loss vs. temperature curve (TG) and derivative (DTG); onset temperature (Tonset), peak decomposition temperature (Tpeak), and residual mass (%)
  • DSC Sample: 5–10 mg in sealed aluminium pan with pierced lid
  • DSC Conditions: N₂ purge (50 mL/min); heating rate 10–20 °C/min; temperature range: 50–400 °C
  • DSC Output: Endothermic peak temperature (Tpeak) and enthalpy of decomposition (ΔH, J/g); pure KELUM® Al(OH)₃ shows a single sharp endotherm at 300–320 °C with ΔH ~1,050 J/g
  • Combined TGA-DSC: Simultaneous thermal analysis (STA) provides correlated mass loss and heat flow data in a single run

4. Performance Data — KELUM® Grades in Polymer Matrices

The table below summarizes typical flame retardant performance results for KELUM® AH-A (ultrafine), AH-B (standard), and AH-C (low-conductivity) grades at 60 wt% loading in EVA, PE, and PVC matrices. All tests were conducted on compression-molded plaques (3.0 mm thickness) conditioned per applicable standards.

KELUM® Grade Matrix (60 wt%) UL 94 Rating
(3.0 mm)
LOI
(% O₂)
Peak HRR
(kW/m² @ 35 kW/m²)
THR
(MJ/m²)
SEA (avg.)
(m²/kg)
Tonset
(°C, TGA)
Char Residue
(% @ 600°C)
AH-A (Ultrafine) EVA (VA 28%) V-0 29.5 185 62 210 252 38.5
AH-A (Ultrafine) LDPE V-0 28.0 220 70 260 255 37.8
AH-A (Ultrafine) PVC (flexible) V-0 32.0 155 48 175 248 40.2
AH-B (Standard) EVA (VA 28%) V-0 28.5 210 68 240 250 38.0
AH-B (Standard) LDPE V-0 27.5 250 76 290 253 37.5
AH-B (Standard) PVC (flexible) V-0 31.0 170 52 195 247 39.8
AH-C (Low Conductivity) EVA (VA 28%) V-0 29.0 195 65 225 251 38.2
AH-C (Low Conductivity) PE (XLPE cable) V-0 28.2 215 71 245 254 37.9

Test conditions: Compression-molded 3.0 mm plaques. 60 wt% KELUM® loading unless otherwise noted. Cone data at 35 kW/m² irradiance, horizontal orientation. All values are typical and may vary with specific formulation (co-additives, processing conditions, specimen thickness). For grade-specific Certificates of Analysis (COA) or formulation optimization support, contact our technical team.

Key observations: AH-A (ultrafine d50 ~1.25 μm) consistently delivers the best balance of flame retardancy and smoke suppression due to superior dispersion in the polymer matrix. AH-C grade maintains flame performance while achieving < 50 μS/cm conductivity — essential for high-voltage cable insulation. All KELUM® grades achieve UL 94 V-0 at 60% loading with LOI values well above the 21% air threshold, confirming excellent self-extinguishing behavior.


5. Custom Testing & Formulation Support

We Test Your Formulation — At No Charge

Hanzhong Delike New Materials Co., Ltd. offers complimentary customer-specific flame retardant testing for qualified prospects and partners. Send us your base polymer (EVA, PE, PP, PVC, PA, rubber, epoxy, or others), and our in-house laboratory will:

Typical turnaround time is 5–7 business days from receipt of your resin sample. We also offer surface-modified grades (AH-SM) for enhanced compatibility and dispersion in polyolefins, engineering thermoplastics, and thermoset composites.

✉
Email
sales@alh3o3.com
☏
Phone
+86-916-2265xxx
(Technical Support)
⌂
Address
Putuo Industrial Park, Hantai District
Hanzhong, Shaanxi, China